Aerospace Materials: MP35N BAR CW-AGED
Aerospace material mechanical properties and design allowables at ambient, elevated, and cryogenic temperatures per MMPDS-11 (Metallic Materials Properties Development and Standardization). Covers primary structural alloys: aluminum (2024-T3, 7075-T6, 6061-T6, 2219-T87), titanium (Ti-6Al-4V), nickel superalloys (Inconel 718), and steels (300M, 4130, 4340).
| material id | temp f | E Msi (Msi) | Fsu ksi (ksi) | Ftu ksi (ksi) | Fty ksi (ksi) | G Msi (Msi) | basis | condition | density lb in3 (lb/in^3) | elongation pct (%) | form | reduction area pct | specification | thickness range |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| MP35N BAR CW-AGED 0.801-1.000 S | 70 | 34 | 145 | 260 | 230 | 11.7 | S | Solution treated, cold drawn, and aged | 0.304 | 8 | Bar | 35 | AMS 5845 | 0.801-1.000 |
| MP35N BAR CW-AGED 1.001-1.750 S | 70 | 34 | — | 260 | 230 | 11.7 | S | Solution treated, cold drawn, and aged | 0.304 | 8 | Bar | 35 | AMS 5845 | 1.001-1.750 |
| MP35N BAR CW-AGED LE0.800 A | 70 | 34 | 145 | 260 | 230 | 11.7 | A | Solution treated, cold drawn, and aged | 0.304 | 8 | Bar | 35 | AMS 5845 | <=0.800 |
| MP35N BAR CW-AGED LE0.800 B | 70 | 34 | 147 | 275 | 266 | 11.7 | B | Solution treated, cold drawn, and aged | 0.304 | — | Bar | — | AMS 5845 | <=0.800 |
What else is in Engineering Database
AI built for engineering. Searches the engineering database, performs calculations, gives source-backed engineering insights.
Get started for free ↗Reference Data375 engineering tablesMaterial properties, pipe and shape dimensions, code tables, and electrical ratings across mechanical, civil, chemical, electrical, materials, and manufacturing engineering.
Browse dataCalculatorsDeterministic engineering calculatorsSizing, checking, and conversion tools that run against the reference tables. Inputs are code-compliant, outputs are traceable to the source standard.
Browse calculators