Explore the Engineering Database more efficiently by signing up for free. Sign up free

Pewter-Sn7Sb2Cu — Tin Alloy

Category
Tin Alloy
Material Id
Pewter Sn7Sb2Cu
Brinell Hardness (HB)
15
Cte per K (1/K)
0.000023
Density Kg M3 (kg/m3)
7,300
Elastic Modulus MPa (MPa)
47,000
Elongation Percent (%)
35
Grade
Britannia/traditional Pewter
Heat Treatment
Cast Or Wrought
Melting Point C (°C)
265
Name
Pewter (Sn-7Sb-2Cu) Traditional
Specific Heat J kgK (J/(kg·K))
230
Standard
CRC Handbook of Chemistry and Physics
Tensile Strength MPa (MPa)
55
Thermal Conductivity W mK (W/(m·K))
50
Yield Strength MPa (MPa)
25

Source: CRC Handbook of Chemistry and Physics

tin_alloy — material id Pewter_Sn7Sb2Cu · name Pewter (Sn-7Sb-2Cu) traditional · grade Britannia/traditional pewter · brinell hardness 15 HB · melting point C 265 °C | Metal Alloy Properties | Engineering Database