Sample data from Engineering Database — 375 reference tables, deterministic calculators, and Engineering AI. Sign up free

Composite Material Properties: AS4 PR 500

CTD -75F A mean to RTW 72F W mean

Fiber-reinforced composite lamina (ply-level) mechanical properties from CMH-17 Rev G, MIL-HDBK-17, and authoritative datasheets. Covers carbon/epoxy, glass/epoxy, aramid/epoxy, PEEK thermoplastic, metal matrix composites (MMC), and ceramic matrix composites (CMC). Properties include elastic constants (E1, E2, G12, nu12), strengths (Xt, Xc, Yt, Yc, S), and physical properties across multiple test conditions (RTD, CTD, ETD, ETW) with mean and B-basis values.

Aerospace Engineeringmaterial system: AS4 PR 50010 rows
material systemcondition basisE1 GPa (GPa)G12 GPa (GPa)S MPa (MPa)Xc MPa (MPa)Xt MPa (MPa)basiscategorydensity kg m3 (kg/m3)fibermatrixply thickness mm (mm)source pagesource tabletest condition
AS4 PR 500CTD -75F A mean61.0195.778723.95meanCarbon Composite1,570AS4PR 5000.3531259; 262Table 4.2.26(d); Table 4.2.26(g)CTD (-75F/A)
AS4 PR 500ETD 180F A mean61.9843.53766.19792.897meanCarbon Composite1,570AS4PR 5000.3493256; 259; 262; 265Table 4.2.26(a); Table 4.2.26(d); Table 4.2.26(g); Table 4.2.26(j)ETD (180F/A)
AS4 PR 500ETD 240F A mean65.7072.979710.16806.687meanCarbon Composite1,570AS4PR 5000.3531256; 260; 262Table 4.2.26(a); Table 4.2.26(e); Table 4.2.26(g)ETD (240F/A)
AS4 PR 500ETD 300F A mean65.5692.48946.884552.27765.318meanCarbon Composite1,570AS4PR 5000.3493257; 260; 262; 265Table 4.2.26(b); Table 4.2.26(e); Table 4.2.26(g); Table 4.2.26(j)ETD (300F/A)
AS4 PR 500ETD 350F A mean62.5351.737351.633723.95meanCarbon Composite1,570AS4PR 5000.3531257; 260; 263Table 4.2.26(b); Table 4.2.26(e); Table 4.2.26(h)ETD (350F/A)
AS4 PR 500ETW 180F W mean66.8793.48955.158689.476772.213meanCarbon Composite1,570AS4PR 5000.3493257; 261; 263; 265Table 4.2.26(b); Table 4.2.26(f); Table 4.2.26(h); Table 4.2.26(j)ETW (180F/W)
AS4 PR 500ETW 240F W mean64.9492.758534.344751.529meanCarbon Composite1,570AS4PR 5000.3531258; 261; 263Table 4.2.26(c); Table 4.2.26(f); Table 4.2.26(h)ETW (240F/W)
AS4 PR 500ETW 300F W mean63.7081.6237.714461.949703.265meanCarbon Composite1,570AS4PR 5000.3493258; 261; 263; 265Table 4.2.26(c); Table 4.2.26(f); Table 4.2.26(h); Table 4.2.26(j)ETW (300F/W)
AS4 PR 500RTD 72F A mean61.2254.40679.979813.581792.897meanCarbon Composite1,570AS4PR 5000.3493256; 259; 262; 265Table 4.2.26(a); Table 4.2.26(d); Table 4.2.26(g); Table 4.2.26(j)RTD (72F/A)
AS4 PR 500RTW 72F W mean4.592meanCarbon Composite1,570AS4PR 5000.3531264Table 4.2.26(i)RTW (72F/W)

What else is in Engineering Database