70-2014-Forging-T652-2.001-3.000-S — 2014 Forging T652

Material Id
2014 Forging T652 2.001-3.000 S
Temp F
70
E Msi (Msi)
10.5
Ec Msi (Msi)
10.8
Fbru Ksi (ksi)
87
Fbru Ksi 2 (ksi)
113
Fbry Ksi (ksi)
76
Fbry Ksi 2 (ksi)
89
Fcy Ksi (ksi)
56
Fcy Ksi Lt (ksi)
56
Fcy Ksi St (ksi)
57
Fsu Ksi (ksi)
37
Ftu Ksi (ksi)
64
Ftu Ksi Lt (ksi)
64
Ftu Ksi St (ksi)
62
Fty Ksi (ksi)
56
Fty Ksi Lt (ksi)
55
Fty Ksi St (ksi)
52
G Msi (Msi)
4
Basis
S
Condition
T652b
Density Lb IN3 (lb/in^3)
0.101
Elongation Pct (%)
8
Elongation Pct Lt (%)
3
Elongation Pct St (%)
2
Form
Hand Forging
Poisson Ratio
0.33
Specification
AMS-a-22771 and AMS-Qq-a-367
Thickness Range
2.001-3.000