Metal Alloy Properties: stainless steel
ATI 321 Annealed to ATI 412 Annealed
Metal and alloy mechanical properties — tensile/yield strength, elastic modulus, density, hardness for steels, aluminum alloys, copper alloys, titanium, nickel alloys, cast iron, and more
| category | material id | brinell hardness (HB) | cte per K (1/K) | density kg m3 (kg/m3) | elastic modulus MPa (MPa) | elongation percent (%) | grade | heat treatment | melting point C (°C) | name | property basis | rockwell b hardness (HRB) | specific heat J kgK (J/(kg·K)) | standard | tensile strength MPa (MPa) | test direction | thermal conductivity W mK (W/(m·K)) | yield strength MPa (MPa) |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| stainless steel | ATI 321 Annealed | 217 | 0.000017 | 7,920 | 193,000 | 40 | 321 | Annealed | 1,398 | ATI 321 Austenitic Stainless Steel (Ti-stabilized) | Minimum | — | 460 | ASTM A240 | 515 | — | 16.3 | 205 |
| stainless steel | ATI 332Mo Annealed | — | 0.000015 | 8,130 | 200,000 | 40 | 332Mo | Annealed | — | ATI 332Mo Austenitic Stainless Steel (High Ni, Automotive Exhaust) | Typical | — | — | ASTM A240 | 585 | — | — | 240 |
| stainless steel | ATI 334Mo Annealed | — | 0.000015 | 7,930 | 200,000 | 50 | 334Mo | Annealed | — | ATI 334Mo Austenitic Stainless Steel (Lean Ni, Automotive Exhaust) | Typical | — | — | ASTM A240 | 565 | — | — | 260 |
| stainless steel | ATI 347 Annealed | 201 | 0.000017 | 7,960 | 193,000 | 40 | 347 | Annealed | 1,398 | ATI 347 Austenitic Stainless Steel (Nb+Ta stabilized) | Minimum | — | 460 | ASTM A240 | 515 | — | 16.3 | 205 |
| stainless steel | ATI 348 Annealed | 201 | 0.000017 | 7,960 | 193,000 | 40 | 348 | Annealed | 1,398 | ATI 348 Austenitic Stainless Steel (Nb+Ta stabilized, Nuclear Grade) | Minimum | — | 460 | ASTM A240 | 515 | — | 16.3 | 205 |
| stainless steel | ATI 409Cb Annealed | — | 0.000011 | 7,760 | 200,000 | 33 | UNS S40945 | Annealed | — | ATI 409Cb Ferritic Stainless Steel | Typical | — | 477 | ASTM A240/A240M | 434 | Longitudinal | 25 | 241 |
| stainless steel | ATI 409HP Annealed | — | 0.000011 | 7,760 | 200,000 | 33 | UNS S40900/S40930 | Annealed | — | ATI 409HP Ferritic Stainless Steel | Typical | 71 | 477 | ASTM A240/A240M | 434 | Longitudinal | 25 | 241 |
| stainless steel | ATI 410S Annealed Minimum | — | — | 7,730 | — | 22 | UNS S41008 | Annealed | — | ATI 410S Ferritic Stainless Steel (ASTM Minimum) | Minimum | — | — | ASTM A240 | 415 | Longitudinal | — | 205 |
| stainless steel | ATI 410S Annealed Typical | — | 0.000011 | 7,730 | 200,000 | 33 | UNS S41008 | Annealed | — | ATI 410S Ferritic Stainless Steel | Typical | 75 | 460 | ASTM A240 | 444 | Longitudinal | 26.9 | 290 |
| stainless steel | ATI 412 Annealed | — | — | 7,750 | — | 24 | UNS S41003 | Sub-critical Anneal | — | ATI 412 Dual-Phase Stainless Steel | Typical | 87 | — | ASTM A240 | 565 | Longitudinal | — | 414 |
What else is in Engineering Database
Iron Engine ↗Engineering AI at ironengine.ai
AI built for engineering. Searches the engineering database, performs calculations, gives source-backed engineering insights.
Get started for free ↗Reference Data375 engineering tablesMaterial properties, pipe and shape dimensions, code tables, and electrical ratings across mechanical, civil, chemical, electrical, materials, and manufacturing engineering.
Browse dataCalculatorsDeterministic engineering calculatorsSizing, checking, and conversion tools that run against the reference tables. Inputs are code-compliant, outputs are traceable to the source standard.
Browse calculators