Waspaloy-Aged — Nickel Alloy

Category
Nickel Alloy
Material Id
Waspaloy Aged
Cte per K (1/K)
0.000013
Density Kg M3 (kg/m3)
8,190
Elastic Modulus MPa (MPa)
211,000
Electrical Resistivity uOhm M (uOhm*m)
1.23
Elongation Percent (%)
28
Grade
N07001
Heat Treatment
Solution Treated 1080C/4h AC + Stabilize 843C/4h AC + Age 760C/16h AC
Melting Point C (°C)
1,360
Name
Waspaloy (Ni-20Cr-14Co-4Mo-3Ti-1.4Al) Aged
Property Basis
Typical
Reduction Percent (%)
49
Specific Heat J kgK (J/(kg·K))
520
Standard
Special Metals Corp. Tech Bulletin Waspaloy (SMC-080); High Temp Metals Waspaloy Tech Data Sheet
Tensile Strength MPa (MPa)
1,427
Thermal Conductivity W mK (W/(m·K))
11
Yield Strength MPa (MPa)
1,041

Source: Special Metals Corp. tech bulletin Waspaloy (SMC-080); High Temp Metals Waspaloy tech data sheet

nickel_alloy — material id Waspaloy_Aged · name Waspaloy (Ni-20Cr-14Co-4Mo-3Ti-1.4Al) aged · grade N07001 · tensile strength MPa 1427 MPa · yield strength MPa 1041 MPa | Metal Alloy Properties | Engineering Database