Sample data from Engineering Database — 375 reference tables, deterministic calculators, and Engineering AI. Sign up free

Insulation R Values: nbs gum rubber

1160 to 1648

Insulation R-values and thermal conductivity data from NIST SRD 81 — covers fiberglass, foam, cellulose, mineral wool, and other building insulation materials

Civil Engineeringmaterial id: nbs gum rubber8 rows
material idrecord iddatedelta t (F)delta x (in)density (lb/ft3)descriptionformk w mk (W/mK)manufacturermaterialmean temp (F)r value per inch (ft2hF/BTU/in)rsi per inch (m2K/W/in)standardtest method
nbs gum rubber11608/11/19597.980.322559.49Natural rubber, ASTM P15-58T: Natural Rubber (100.0), Zinc Oxide (6.0), Sulphur (3.5), Stearic Acid (0.5), Mercaptobenzo-thiozole (0.5).Slab0.998NBS, Leather SectionNBS Gum Rubber115.650.1445170.025451NIST SRD 81 APIASTM C 177
nbs gum rubber15286/5/196411.130.486660.84Natural rubber, ASTM-2A recipe, cure 140 °C, 0.5 h: R(100g); ZnO(5g); S(2.5g); Stearic acid(2.0g); Altex(1.0g); phenyl beta naphthylamine (antioxidant) (1.0g); Samples 8x8x½ in., No.1,6Slab1.0331NBS, Rubber SectionNBS Gum Rubber129.760.1396070.024586NIST SRD 81 APIASTM C 177
nbs gum rubber15296/8/196410.830.47861.93Natural rubber, ASTM-2A recipe, cure 140 °C, 0.5 h: R(100g); ZnO(5g); S(2.5g); Stearic acid(2.0g); Altex(1.0g); phenyl beta naphthylamine (antioxidant) (1.0g); Samples 8x8x½ in., No.1,6Slab1.0393NBS, Rubber SectionNBS Gum Rubber69.670.1387740.02444NIST SRD 81 APIASTM C 177
nbs gum rubber15306/9/196410.660.472262.69Natural rubber, ASTM-2A recipe, cure 140 °C, 0.5 h: R(100g); ZnO(5g); S(2.5g); Stearic acid(2.0g); Altex(1.0g); phenyl beta naphthylamine (antioxidant) (1.0g); Samples 8x8x½ in., No.1,6Slab1.0406NBS, Rubber SectionNBS Gum Rubber18.460.1386010.024409NIST SRD 81 APIASTM C 177
nbs gum rubber15386/30/196410.530.478261.75Natural rubber, ASTM-2A recipe, cure 140 °C, 0.5 h: R(100g); ZnO(5g); S(2.5g); Stearic acid(2.0g); Altex(1.0g); phenyl beta naphthylamine (antioxidant) (1.0g); Samples 8x8x½ in., No.1,6Slab1.0636NBS, Rubber SectionNBS Gum Rubber70.40.1356040.023881NIST SRD 81 APIASTM C 177
nbs gum rubber15397/1/196410.560.479861.83Natural rubber, ASTM-2A recipe, cure 140 °C, 0.5 h: R(100g); ZnO(5g); S(2.5g); Stearic acid(2.0g); Altex(1.0g); phenyl beta naphthylamine (antioxidant) (1.0g); Samples 8x8x½ in., No.1,6Slab1.0652NBS, Rubber SectionNBS Gum Rubber70.440.13540.023845NIST SRD 81 APIASTM C 177
nbs gum rubber15407/2/196420.650.962861.56Natural rubber, ASTM-2A recipe, cure 140 °C, 0.5 h: R(100g); ZnO(5g); S(2.5g); Stearic acid(2.0g); Altex(1.0g); phenyl beta naphthylamine (antioxidant) (1.0g); Samples 8x8x½ in., No.1,6Slab1.0517NBS, Rubber SectionNBS Gum Rubber72.180.1371380.024151NIST SRD 81 APIASTM C 177
nbs gum rubber16483/28/196618.550.685461.85Natural rubber, ASTM-2A recipe, cure 140 °C, 0.5 h: R(100g); ZnO(5g); S(2.5g); Stearic acid(2.0g); Altex(1.0g); phenyl beta naphthylamine (antioxidant) (1.0g); Samples 8x8x3/4 in., No. 1,3,5 & 2,4,6Slab1.0487NBS, Rubber SectionNBS Gum Rubber70.150.137530.02422NIST SRD 81 APIASTM C 177