Explore the Engineering Database more efficiently by signing up for free. Sign up free

Biir — Iir

Elastomer
Iir
Grade Or Variant
Biir
Acid Resistance
Excellent
ASTM Designation
AA, Ba (ASTM D2000)
Chemical Resistance Notes
Same As CIIR; Bromine Functionality Enables Faster Cure and Better Co-Cure compatibility; Slightly Better Adhesion to Metals and Fabrics
Common Name
Bromobutyl Rubber
Compression Set Pct (%)
25-50
Compression Set Temp C
100
Compression Set Time Hr
22
Cure System
sulfur, resin, Zinc oxide, Or Peroxide
Density G CM3 (g/cm3)
1.15-1.35
Elongation at Break Pct (%)
400-800
Fuel Resistance
Poor
Gas Permeability
Very Low
Glass Transition Temp C (C)
-70
Hardness Range Shore a
35-95
Max Continuous Temp C (C)
130
Max Peak Temp C (C)
150
Max Service Temp C (C)
130
Min Service Temp C (C)
-50
Oil Resistance
Poor
Ozone Resistance
Excellent
Steam Resistance
Good
Tensile Strength Mpa (MPa)
7-17
IIR — grade or variant BIIR · chemical resistance notes Same as CIIR; bromine functionality enables faster cure and better co-cure… · common name Bromobutyl Rubber · max continuous temp C 130 C · max service temp C 130 C | Elastomer Service Properties | Engineering Database