Explore the Engineering Database more efficiently by signing up for free. Sign up free
Home/Reference Data/Aerospace Materials/7075 Forging T6/70-7075-FORGING-T6-LE2.000-S-T3-7-6-0f1-C5

70-7075-Forging-T6-LE2.000-S-T3-7-6-0F1-C5 — 7075 Forging T6

Material Id
7075 Forging T6 LE2.000 S T3 7 6 0F1 C5
Temp F
70
E Msi (Msi)
10
Ec Msi (Msi)
10.4
Fsu Ksi (ksi)
41
Ftu Ksi (ksi)
68
Ftu Ksi Lt (ksi)
66
Ftu Ksi St (ksi)
65
Fty Ksi (ksi)
56
Fty Ksi Lt (ksi)
55
Fty Ksi St (ksi)
55
G Msi (Msi)
3.8
Basis
S
Condition
T6a
Density Lb IN3 (lb/in^3)
0.101
Elongation Pct (%)
6
Elongation Pct Lt (%)
3
Elongation Pct St (%)
2
Form
Hand Forging
Poisson Ratio
0.33
Specification
AMS 4126, AMS-a-22771, and AMS-Qq-a-367
Thickness Range
<=2.000