Explore the Engineering Database more efficiently by signing up for free. Sign up free

70-2014-Forging-T6-LE2.000-S — 2014 Forging T6

Material Id
2014 Forging T6 LE2.000 S
Temp F
70
E Msi (Msi)
10.5
Ec Msi (Msi)
10.8
Fbru Ksi (ksi)
91
Fbru Ksi 2 (ksi)
117
Fbry Ksi (ksi)
78
Fbry Ksi 2 (ksi)
90
Fcy Ksi (ksi)
56
Fcy Ksi Lt (ksi)
56
Fsu Ksi (ksi)
40
Ftu Ksi (ksi)
65
Ftu Ksi Lt (ksi)
65
Fty Ksi (ksi)
56
Fty Ksi Lt (ksi)
56
G Msi (Msi)
4
Basis
S
Condition
T6a
Density Lb IN3 (lb/in^3)
0.101
Elongation Pct (%)
8
Elongation Pct Lt (%)
3
Form
Hand Forging
Poisson Ratio
0.33
Specification
AMS 4133, AMS-a-22771, and AMS-Qq-a-367
Thickness Range
<=2.000