Material Id
2014 Forging T6 6.001-7.000 S
Temp F
70
E Msi (Msi)
10.5
Ec Msi (Msi)
10.8
Ftu Ksi (ksi)
60
Ftu Ksi Lt (ksi)
60
Ftu Ksi St (ksi)
58
Fty Ksi (ksi)
52
Fty Ksi Lt (ksi)
52
Fty Ksi St (ksi)
52
G Msi (Msi)
4
Basis
S
Condition
T6a
Density Lb IN3 (lb/in^3)
0.101
Elongation Pct (%)
6
Elongation Pct Lt (%)
2
Elongation Pct St (%)
1
Form
Hand Forging
Poisson Ratio
0.33
Specification
AMS 4133, AMS-a-22771, and AMS-Qq-a-367
Thickness Range
6.001-7.000