Part of Engineering Database. 375 reference tables, deterministic calculators, and Engineering AI. Sign up free
Home/Compare/Nickel Alloy/Inconel 617 (Ni-22Cr-12Co-9Mo) annealed vs Inconel 718

Inconel 617 (Ni-22Cr-12Co-9Mo) annealed vs Inconel 718

Property comparison of Inconel 617 (Ni-22Cr-12Co-9Mo) annealed and Inconel 718, both nickel alloy.

Nickel Alloy10 compared properties
PropertyInconel 617 (Ni-22Cr-12Co-9Mo) annealedInconel 718Difference
Yield strength330 MPa1,036 MPa+214%
Tensile strength740 MPa1,240 MPa+68%
Elongation55 %12 %-78%
Elastic modulus211,000 MPa211,000 MPa0%
Density8,360 kg/m³8,220 kg/m³-2%
Brinell hardness170 HB331 HB+95%
Thermal conductivity13.4 W/m·K11.4 W/m·K-15%
Specific heat419 J/kg·K435 J/kg·K+4%
Coefficient of thermal expansion0.000013 1/K0.000013 1/K+2%
Melting point1,380 °C1,336 °C-3%

Difference is Inconel 718 relative to Inconel 617 (Ni-22Cr-12Co-9Mo) annealed. Values are taken from the representative row of each material; both materials may have multiple heat treatments or conditions on their individual pages.

Identification

Inconel 617 (Ni-22Cr-12Co-9Mo) annealed
grade
N06617
standard
Special Metals Corp. tech bulletin INCONEL alloy 617 (SMC-029)
heat treatment
solution-annealed
Inconel 718
grade
N07718
standard
Special Metals Corp. tech bulletin INCONEL alloy 718 (SMC-045); AMS 5663
heat treatment
solution annealed + double aged (720C/8h + 620C/8h)

About Inconel nickel-chromium superalloys

Inconel is a family of nickel-chromium-iron superalloys. They keep strength at temperatures where steels and most stainless grades have failed and resist oxidation and hot corrosion. Inconel 718 is the most widely used grade for aerospace turbine disks and high-temperature fasteners; Inconel 625 is the choice when chloride and reducing-acid corrosion both matter.