Explore the Engineering Database more efficiently by signing up for free. Sign up free
Al-2219-T87-L-195K — Aluminum Alloy
- Category
- Aluminum Alloy
- Material Id
- Al 2219 T87 L 195K
- Cte per K (1/K)
- 0.000021
- Density Kg M3 (kg/m3)
- 2,820
- Elastic Modulus MPa (MPa)
- 81,200
- Elongation Percent (%)
- 13.35
- Grade
- 2219-T87
- Heat Treatment
- T87
- Name
- Al 2219-T87 Longitudinal
- Poisson Ratio (dimensionless)
- 0.325
- Property Basis
- Typical
- Reduction Percent (%)
- 27.85
- Shear Modulus MPa (MPa)
- 30,600
- Specific Heat J kgK (J/(kg·K))
- 736
- Standard
- Nistir 3971
- Tensile Strength MPa (MPa)
- 496.75
- Test Direction
- Longitudinal
- Test Temperature C (C)
- -78.15
- Thermal Conductivity W mK (W/(m·K))
- 100
- Yield Strength MPa (MPa)
- 409
Source: NISTIR 3971