Explore the Engineering Database more efficiently by signing up for free. Sign up free

Etw-180F-W-Mean — Celion 12K 938

Material System
Celion 12K 938
Condition Basis
Etw 180F W Mean
E1 GPa (GPa)
125.485
E2 GPa (GPa)
8.205
S MPa (MPa)
96.527
Vf Pct (%)
61.5
Xc MPa (MPa)
1,275.53
Xt MPa (MPa)
1,909.848
Yt MPa (MPa)
39.99
Basis
Mean
Density Kg M3 (kg/m3)
1,590
Fiber
Celion 12K
Matrix
938
NU12 (dimensionless)
0.345
Ply Thickness MM (mm)
0.1372
Source Page
128; 129; 131; 132
Source Table
Table 4.2.7(B); Table 4.2.7(C); Table 4.2.7(E); Table 4.2.7(F)
Test Condition
Etw (180F/W)