70-Inconel-X750-Bar-Forging-Eq-Aged-4.000-10.000-S — Inconel X750 Bar Forging Eq Aged
- Material Id
- Inconel X750 Bar Forging Eq Aged 4.000-10.000 S
- Temp F
- 70
- E Msi (Msi)
- 30.6
- Ec Msi (Msi)
- 30.6
- Fbru Ksi (ksi)
- 240
- Fbru Ksi 2 (ksi)
- 304
- Fbry Ksi (ksi)
- 150
- Fbry Ksi 2 (ksi)
- 180
- Fcy Ksi (ksi)
- 100
- Fsu Ksi (ksi)
- 99
- Ftu Ksi (ksi)
- 160
- Fty Ksi (ksi)
- 100
- G Msi (Msi)
- 11.8
- Ra Pct (%)
- 17
- Basis
- S
- Condition
- Equalized and Aged
- Density Lb IN3 (lb/in^3)
- 0.298
- Elongation Pct (%)
- 15
- Form
- Bars and Forgings
- Poisson Ratio
- 0.3
- Specification
- AMS 5667
- Thickness Range
- 4.000-10.000