Ti-6Al-2Fe-0.1Si (TIMETAL 62S) Annealed vs Ti-6Al-2Sn-4Zr-2Mo Forging STA (Duplex Annealed)
Property comparison of Ti-6Al-2Fe-0.1Si (TIMETAL 62S) Annealed and Ti-6Al-2Sn-4Zr-2Mo Forging STA (Duplex Annealed), both titanium alloy.
| Property | Ti-6Al-2Fe-0.1Si (TIMETAL 62S) Annealed | Ti-6Al-2Sn-4Zr-2Mo Forging STA (Duplex Annealed) | Difference |
|---|---|---|---|
| Yield strength | 896 MPa | 827.4 MPa | -8% |
| Tensile strength | 930 MPa | 896.3 MPa | -4% |
| Elongation | 10 % | 10 % | 0% |
| Elastic modulus | 128,000 MPa | 113,764 MPa | -11% |
| Density | 4,440 kg/m³ | 4,540 kg/m³ | +2% |
Difference is Ti-6Al-2Sn-4Zr-2Mo Forging STA (Duplex Annealed) relative to Ti-6Al-2Fe-0.1Si (TIMETAL 62S) Annealed. Values are taken from the representative row of each material; both materials may have multiple heat treatments or conditions on their individual pages.
Identification
- grade
- Ti-6Al-2Fe-0.1Si
- standard
- Mil-T-9047 / AMS Provisional
- heat treatment
- Annealed
- grade
- Ti-6Al-2Sn-4Zr-2Mo
- standard
- MIL-HDBK-5J
- heat treatment
- Solution Treated and Aged (Duplex Annealed)
What else is in Engineering Database
AI built for engineering. Searches the engineering database, performs calculations, gives source-backed engineering insights.
Get started for free ↗Reference Data375 engineering tablesMaterial properties, pipe and shape dimensions, code tables, and electrical ratings across mechanical, civil, chemical, electrical, materials, and manufacturing engineering.
Browse dataCalculatorsDeterministic engineering calculatorsSizing, checking, and conversion tools that run against the reference tables. Inputs are code-compliant, outputs are traceable to the source standard.
Browse calculators